Home News

Tracking Test: 175 V, Fifty Drops and the Carbon Path That Forms

Tracking Test: 175 V, Fifty Drops and the Carbon Path That Forms

Good quality IEC 60065 Standard for sales
Good quality IEC 60065 Standard for sales
Our goods has safely arrived at our residence. Thank you for your excellent services. I hope we can cooperate again in the future.

—— Wira

I'm Online Chat Now
Tracking Test: 175 V, Fifty Drops and the Carbon Path That Forms

Tracking is the failure mode where a conductive path forms across the surface of an insulator. It starts as a localised burn at a point of high current density, carbonises the surface, and the carbon makes the next event worse. The tracking test reproduces that in a controlled way, and the number of drops to failure is the result.

What the test does

Two electrodes rest on the specimen surface at a defined spacing. A conductive solution — ammonium chloride in water — is dripped between them at a defined rate. A voltage is applied, and the test continues until a path forms or the drop count reaches a limit.

The result is expressed either as the number of drops at which tracking occurs, or as the voltage at which a material survives a specified number of drops. The comparative tracking index, CTI, is the voltage at which a material withstands 50 drops without tracking.

QuantityMeaningTypical use
CTIvoltage for 50 dropsmaterial selection, grouping
proof tracking indexvoltage survived by all specimensqualification

Why the drop count matters

Tracking is a cumulative process. Each drop evaporates and concentrates the salt, each event heats the surface, and the damage accumulates. A material that fails after 20 drops is not the same as one that fails after 200, even if both fail at the same voltage.

This is why the drop count is part of the result and not just a procedure detail. Quoting "failed at 200 V" without the drop count describes half the finding.

Why the surface condition dominates

Tracking is a surface phenomenon, so anything on the surface changes the result:

Contamination. Mould release agent, handling oils, dust — all change how the solution wets the surface and where it pools. A moulded part straight from the tool behaves differently from one that has been handled.

Surface finish. A rougher surface holds the solution in place and produces a longer wet path; a polished surface lets it run off. The standard specifies the specimen preparation, and deviating from it produces a different test.

Geometry. A rib between the electrodes changes the path length. A part tested as a flat plaque and then used with a rib has not been tested in its real configuration.

What tracking looks like when it starts

The first sign is a small sparking at one electrode, often with a visible glow. Then a dark spot appears on the surface, and it grows. Once carbon is present, the resistance drops, the current concentrates, and the process accelerates.

Burning may continue after the voltage is removed if the material sustains combustion — that is a different failure mode, and it is judged separately.

Interpreting a marginal result

A material that tracks at 175 V and is used at 250 V has no margin. A material that survives 50 drops at 400 V in the lab may track in service if the surface is contaminated with something more conductive than the test solution — salt spray, for instance.

The test gives a comparison between materials under defined conditions. It does not give a service voltage rating, and treating it as one is how products pass type testing and fail in the field.

What to record

Voltage, drop rate, solution concentration, electrode spacing and force, specimen thickness and surface preparation, and the drop count at failure. For a CTI determination, the number of specimens and the statistical treatment matter as much as the individual results.

A single specimen result is an observation. A CTI value is a statement about a material, and it needs the sample size to support it.