Home News

Glow-Wire Test: 960 °C, 30 Seconds and the Part That Keeps Burning

Glow-Wire Test: 960 °C, 30 Seconds and the Part That Keeps Burning

Good quality IEC 60065 Standard for sales
Good quality IEC 60065 Standard for sales
Our goods has safely arrived at our residence. Thank you for your excellent services. I hope we can cooperate again in the future.

—— Wira

I'm Online Chat Now
Glow-Wire Test: 960 °C, 30 Seconds and the Part That Keeps Burning

The glow-wire test produces the most misunderstood result in safety testing. A part is pressed against a wire heated to 550, 650, 750 or 960 °C for 30 seconds, then removed, and the question is not "did it burn" but "did it stop burning, and did it set anything else alight".

What the test actually asks

Two criteria, evaluated separately:

Ignition. Did the specimen ignite during the 30 seconds of contact? If it did not, the test passes regardless of what happens afterwards.

Flame persistence. If it ignited, did the flame extinguish within 30 seconds after the wire is removed, and did the burning material or the dropping particles ignite a specified layer of tissue paper below?

A part that chars, smokes and melts but never sustains a flame is a pass. A part that produces a small flame which dies in 5 seconds is a pass. A part that looks untouched but drops one glowing particle onto the tissue is a fail.

TemperatureTypical applicationWhat it implies
550 °Cparts unlikely to be contacted by a hot elementlowest severity level
650 °Cparts near but not supporting current-carrying partsmoderate
750 °Cparts supporting live partshigh
960 °Cparts retaining current-carrying connectionshighest

Why the temperature level matters more than the material

Two identical mouldings tested at 750 °C and 960 °C produce different results on the same day. The material has not changed; the question has. This is why "it passed the glow-wire test" is a meaningless statement without the temperature, and why a supplier quoting a pass without a level should be asked again.

The level is chosen by the product standard based on what the part does, not on what the material can survive. A part that holds a terminal block gets 960 °C whether it is made of PBT or polycarbonate.

The setup details that change results

Wire temperature calibration. The wire is heated by current and its temperature is measured by a thermocouple before the test. A wire that reads 960 °C at the start but 920 °C after 30 seconds of contact is not delivering the specified severity. The current must be adjusted to hold the temperature throughout.

Contact force and depth. The wire is pressed 7 mm into the specimen with a force of about 1 N. A shallower penetration tests a different thermal mass and gives a more optimistic result.

Specimen orientation. The test is performed with the specimen in its normal position. A part that was designed to be vertical and tested horizontally behaves differently because the melted material flows away from the wire instead of pooling around it.

Conditioning. Polymeric materials absorb moisture, and a damp specimen behaves differently from a dry one. The standard specifies conditioning, and skipping it is the most common reason for an unrepeatable result.

Reading the result honestly

A glow-wire pass does not mean the part will not burn in a fire. It means the part, in a defined configuration, did not sustain combustion after a defined thermal insult. That is a narrow but useful statement, and it is the one the standard asks for.

The failure that gets argued about most is the tissue-paper ignition. A single glowing droplet that lands on the tissue and chars it is a fail even though the specimen itself stopped burning. Operators who watch only the specimen miss it, which is why the paper layer has to be placed and inspected deliberately rather than left as an afterthought.