Glow Wire at 960 Degrees: Thirty Seconds, Tissue Paper and Two Ways to Fail

Of all the glow-wire temperatures in use, 960 degrees C produces the most discussion and the least agreement. It is the highest temperature in common use under IEC 60695-2-10, it appears in product standards for parts that must not propagate fire, and it has two failure modes that are recorded separately and often collapsed into one.

Where 960 comes from

The glow-wire temperatures form a short list, and product standards pick from it according to how the part is used:

550 degrees CParts that may be touched and are not near a heat source
650 degrees CParts that may be touched, with a modest thermal load
750 degrees CParts that hold current-carrying connections
850 degrees CParts near a source of ignition
960 degrees CParts that must contain a fire, or unattended appliances where the consequence of fire is severe

960 is not "the strictest test" in an absolute sense; it is the temperature applied where the consequence of failure justifies it. Applying it to a part the product standard tests at 650 is not a better test, it is a test the part was never designed for.

The application, in detail

The loop is brought to temperature and held for at least 60 s, then applied to the specimen for 30 s with a force of 1 N. The specimen is mounted as in service, with the tissue paper positioned below at the distance the method specifies.

Three details decide whether the application is the specified one:

  • The 1 N must be real. Friction in the carriage, a stiff specimen holder or a specimen that moves under the load all reduce the effective force. Check with a balance at the specimen plane.
  • The application must be to a defined surface. Testing a flat plaque is not testing a rib. The thinnest section that exists in service is the one that matters.
  • The 30 s starts at contact. A loop that is brought close and then advanced slowly has already transferred heat before the timer starts.

The two failure modes

This is the point most reports miss. A specimen fails in one of two ways, and they are not equivalent:

  1. It sustains flame. After the loop is withdrawn, the specimen continues to burn beyond the time limit defined for the index being determined. This is the obvious failure.
  2. It drops burning material. The specimen may extinguish within the time limit and still fail, because a flaming droplet ignites the tissue paper below. This is the failure that a report recording only "afterflame time" will miss entirely.

A material can have an excellent afterflame performance and a poor droplet behaviour, and the droplet behaviour is often the more relevant one in an enclosure with a wiring harness below the part.

Reading the tissue paper

The tissue paper is not decoration. It is the detector for mode two, and three things affect whether it works:

  • Distance. The paper must be at the specified distance below the specimen. Closer and it ignites from radiant heat; further and a small droplet may not reach it.
  • Condition. Fresh, dry paper. Damp paper will not ignite, and the test becomes easier without anyone noticing.
  • Coverage. The paper must extend beyond the footprint of the specimen in all directions, so a droplet that falls at an angle still lands on it.

What to record

Five items, in this order: test temperature, application time, time to extinguish after withdrawal, whether the tissue paper ignited, and the post-test condition of the specimen including penetration depth and whether the part remains functional.

The last item is the one that turns a test result into an engineering finding. A part that passes both flame criteria but has a hole through a wall that carries a creepage path has failed in the sense that matters to the product standard, and that failure is invisible in the flame data.