Glow Wire: 960, 850 and 650 Degrees Ask Three Different Questions

The glow wire test is often described as a flammability test. It is not, quite. It measures whether a material ignites when pressed against a hot element, and whether it sustains flame afterwards — two different questions with two different answers, and three different standards that ask them separately.

The three variants

The family in IEC 60695-2 covers three related tests, and mixing them up is the most common error in a test report:

Glow wire flammability index (GWFI) — the highest temperature at which a material, pressed against the glowing wire, extinguishes within a defined time after the wire is removed and does not ignite the underlying tissue paper.

Glow wire ignition temperature (GWIT) — the temperature at which the material does not ignite at all during the application, with a defined margin.

Glow wire test (GWT) — a single test at a temperature specified by the product standard, with a pass or fail on ignition, flame duration and burning drops.

TestQuestionResult form
GWFIdoes it stop burning quicklya temperature index
GWITdoes it avoid ignitinga temperature, 25 K below the trial
GWTpass or fail at one temperaturepass or fail

The apparatus is small and specific

A loop of nickel-chromium wire, formed to a defined shape, heated electrically to the test temperature and pressed against the specimen with a defined force for a defined time — commonly 1 N for 30 seconds.

The temperature is measured by a thermocouple in the wire loop, and the calibration of that loop is where most laboratories drift. A loop that has been used many times changes shape, and a changed shape changes the contact area and therefore the heat transfer.

What the result actually says

Three observations are recorded: whether the specimen ignites, how long flame persists after the wire is removed, and whether burning material drips and ignites the tissue below.

The second observation is the one that separates materials most clearly. A material that ignites but extinguishes in two seconds is treated differently from one that burns for thirty, even though both "ignited".

The third observation is about the product, not the material: a dripping thermoplastic can carry fire away from the ignition point and into a region that was never designed for it.

Why 960, 850 and 650

These are the temperatures that appear most often in product standards, and they correspond to severity levels for parts in different positions relative to a source of heat.

960 °C is used for parts that must retain a function during a fault. 850 °C and 650 °C appear for parts where the consequence of ignition is less severe or where the mass of material is small.

The temperature is chosen by the product standard, not by the material supplier, and a material that passes at 960 °C is not automatically acceptable where the standard asks for a specific behaviour at that temperature.

Sample preparation and the thin-wall problem

Specimens are normally plaques of defined thickness. A part moulded at 1.2 mm is not represented by a 3 mm plaque, and thin sections ignite more readily and distort away from the wire.

Where the product has thin walls, the test should be run on specimens of that thickness. A pass on a thicker plaque is evidence about a different object.

What the test does not cover

It does not model a flame. A material that resists a glowing wire can still burn vigorously when exposed to a small flame, which is why the glow wire and the needle flame tests coexist rather than replace each other.

It also does not model long-term thermal degradation. A part that passes at 960 °C when new may be brittle and cracked after years at 100 °C, and the glow wire test says nothing about that.

What to record

Test variant, temperature, force, duration, specimen thickness, ignition, flame duration, dripping, and the loop calibration date. The calibration date is the field that makes two reports comparable, and it is usually the one omitted.