Ball Pressure at 75 °C or 125 °C: Choosing the Temperature for the Part

Of all the fire and heat tests, the ball pressure test has the fewest variables. A 5 mm steel ball, a 20 N load, a specified temperature, one hour, and a measurement of the resulting indentation. The judgement is a diameter, usually 2 mm. Everything that goes wrong with the test goes wrong in the choice of temperature, or in the preparation of the sample.

Where the two temperatures come from

The temperatures are not material properties; they are consequences of the product. A part that is only accessible when the appliance is opened, and that is not near a heat source, is tested at the lower temperature. A part that supports a current-carrying connection, or that is in contact with a part that reaches a high temperature in normal use, is tested higher, because the material has to keep its shape while hot.

The number that drives the choice is the temperature rise measured on that part during the heating test, plus the ambient, plus a margin. A terminal block that reaches 95 °C in a 25 °C room is a 70 K rise, and if the standard requires the ball test at the temperature of the part plus a margin, the part belongs in the higher band, not the lower one.

Part locationMeasured temperature in normal useBall test temperatureTypical indentation limit
Enclosure, not near heat35 to 45 °C75 °C2 mm
Enclosure near a heat source55 to 70 °C75 °C, evaluate separately2 mm
Terminal block, current-carrying70 to 100 °C125 °C2 mm
Support of a live part80 to 110 °C125 °C2 mm
Part in contact with a heating elementAbove 100 °CHigher band, per product standard2 mm

Sample preparation decides the result

A ball pressure test on a 2 mm thick sample cut from a moulding reads differently from the same test on the finished part. The moulding has ribs, a flow pattern, and residual stress; a cut coupon has none of them. The standard asks for the part, or a representative section, and a coupon is only acceptable when the part is too small or too curved to test.

The sample must also be conditioned. A polyamide that has absorbed 2 % moisture softens at a lower temperature than the dry resin, and a test run on a sample straight from a humid store will show a larger indentation than one run after drying. If the material specification is for the dry state, dry the sample; if the part runs wet in service, that is the state to test, and it should be written down.

Reading the indentation

The measurement is the diameter of the impression left by the ball, measured with a travelling microscope or a profile projector, after the sample has cooled. Measuring while hot, or measuring the ball rather than the impression, are both common errors. The impression is not circular if the sample was not level, and an oval impression is a setup problem, not a material result.

  • Sample flat and supported on a rigid plate, not on a soft backing.
  • Ball and sample at the test temperature before the load is applied; a cold ball cools the surface locally.
  • Load applied without impact; a dropped weight is a different test.
  • One hour at temperature, then cool before measuring.
  • Measure across the widest and narrowest axes and report both.

What a marginal result means

A 2.1 mm indentation is a fail, and a 1.9 mm indentation is a pass, but the difference between them is often batch-to-batch variation rather than design. A part that measures 1.8 mm on one batch and 2.1 mm on the next has a process problem: regrind content, mould temperature, or insufficient drying. Looking at the trend over three lots is more informative than the individual verdict.

Standards referenced: IEC 60695-10-2 (ball pressure test), with the test temperature and the indentation limit taken from the relevant product standard (IEC 60335-1, IEC 61010-1, IEC 60598-1).